OK....not really.
But just ran some Lincoln Outershield (flux core, gas shielded) for the first time...and wow am I impressed! This stuff really fuses in hot.
But what I can't seem to find is some recommended settings for .035 wire. I'm on a Lincoln Power Mig 210 so limited in my output - or would be on .045. My books and internet research only turns up settings for .045....and yes I have watched Jodi's videos on dual shield.
Picture below my first attempt...1/4" wall 2x 6 tubing. I know....the crown is a little high...I did bevel it a bit. Settings used were circa 300/22.7v on 75/25 mix.
*Would love some suggestions on hotter settings for 3/8" & 1/2" plate, multiple pass....
Thanks in advance....
mig and flux core tips and techniques, equipment, filler metal
getherdone
- getherdone
-
Active Member
-
Posts:
-
Joined:Sat Feb 20, 2016 10:34 pm
- Attachments
-
- IMG_7281.JPG-2.jpeg (47.06 KiB) Viewed 598 times
Last edited by getherdone on Sun Oct 23, 2016 9:32 am, edited 1 time in total.
Lincoln Power Mig 210MP
Everlast Power TIG 185
Hypertherm PowerMax 45
Everlast Power TIG 185
Hypertherm PowerMax 45
- MinnesotaDave
-
Weldmonger
-
Posts:
-
Joined:Sun Oct 27, 2013 10:57 pm
-
Location:Big Lake/Monticello MN, U.S.A.
In general, to flatten and widen a bead with mig, turn up the voltage.
Dave J.
Beware of false knowledge; it is more dangerous than ignorance. ~George Bernard Shaw~
Syncro 350
Invertec v250-s
Thermal Arc 161 and 300
MM210
Dialarc
Tried being normal once, didn't take....I think it was a Tuesday.
Beware of false knowledge; it is more dangerous than ignorance. ~George Bernard Shaw~
Syncro 350
Invertec v250-s
Thermal Arc 161 and 300
MM210
Dialarc
Tried being normal once, didn't take....I think it was a Tuesday.
getherdone
- getherdone
-
Active Member
-
Posts:
-
Joined:Sat Feb 20, 2016 10:34 pm
Here's the latest....multiple passes with one wide cover pass....
- IMG_7289.JPG.jpeg (41.88 KiB) Viewed 534 times
Lincoln Power Mig 210MP
Everlast Power TIG 185
Hypertherm PowerMax 45
Everlast Power TIG 185
Hypertherm PowerMax 45
Return to “Mig and Flux Core - gas metal arc welding & flux cored arc welding”
Jump to
- Introductions & How to Use the Forum
- ↳ Welcome!
- ↳ Member Introductions
- ↳ How to Use the Forum
- ↳ Moderator Applications
- Welding Discussion
- ↳ Metal Cutting
- ↳ Tig Welding - Tig Welding Aluminum - Tig Welding Techniques - Aluminum Tig Welding
- ↳ Mig and Flux Core - gas metal arc welding & flux cored arc welding
- ↳ Stick Welding/Arc Welding - Shielded Metal Arc Welding
- ↳ Welding Forum General Shop Talk
- ↳ Welding Certification - Stick/Arc Welding, Tig Welding, Mig Welding Certification tests - Welding Tests of all kinds
- ↳ Welding Projects - Welding project Ideas - Welding project plans
- ↳ Product Reviews
- ↳ Fuel Gas Heating
- Welding Tips & Tricks
- ↳ Video Discussion
- ↳ Wish List
- Announcements & Feedback
- ↳ Forum News
- ↳ Suggestions, Feedback and Support
- Welding Marketplace
- ↳ Welding Jobs - Industrial Welding Jobs - Pipe Welding Jobs - Tig Welding Jobs
- ↳ Classifieds - Buy, Sell, Trade Used Welding Equipment
- Welding Resources
- ↳ Tradeshows, Seminars and Events
- ↳ The Welding Library
- ↳ Education Opportunities