After running many beads on plate and getting familiar with the machine controls on my TIG welder. I started working on the cart for it. I feel I have some decent welds but still have lots of room for improvement.
The material is 11 gage 1-1/4 square tube. I was running a 1/16" 2% Lanthated Tungsten ground to a point. Machine was set at 110 amps #8 cup gas lense and 18CFH of argon.
Here are a few pictures for you guys to offer your suggestions.
Brian
Tig welding tips, questions, equipment, applications, instructions, techniques, tig welding machines, troubleshooting tig welding process
- MinnesotaDave
-
Weldmonger
-
Posts:
-
Joined:Sun Oct 27, 2013 10:57 pm
-
Location:Big Lake/Monticello MN, U.S.A.
It's looking very good - in my opinion you're just going to get better and more consistent from here.
Dave J.
Beware of false knowledge; it is more dangerous than ignorance. ~George Bernard Shaw~
Syncro 350
Invertec v250-s
Thermal Arc 161 and 300
MM210
Dialarc
Tried being normal once, didn't take....I think it was a Tuesday.
Beware of false knowledge; it is more dangerous than ignorance. ~George Bernard Shaw~
Syncro 350
Invertec v250-s
Thermal Arc 161 and 300
MM210
Dialarc
Tried being normal once, didn't take....I think it was a Tuesday.
- big gear head
-
Ace
-
Posts:
-
Joined:Thu May 07, 2015 11:46 am
-
Location:KY.
Thanks guys. I find that I am spending more time getting comfortable doing dry runs before i strike an arc than I am welding. By the time I feel I have a nice bead going I'm at the end. Lol. here is another picture. At the termination of all the welds I have a small black spot. Is this normal?
Brian
Brian
Last edited by melsdad on Mon Feb 15, 2016 8:04 pm, edited 1 time in total.
Brian
Miller Thunderbolt 225 AC/DC
Everlast 255EXT with W300 cooler
Hobo Freight 170 MIG Welder
Miller Thunderbolt 225 AC/DC
Everlast 255EXT with W300 cooler
Hobo Freight 170 MIG Welder
- LtBadd
-
Weldmonger
-
Posts:
-
Joined:Sun Apr 12, 2015 4:00 pm
-
Location:Clearwater FL
-
Contact:
Yes, I believe that is silicon floating in the puddle, your bead looks very good and the dry run technique is the way to go. You have to be comfortable to make good welds (typically)melsdad wrote:Thanks guys. I find that I am spending more time getting comfortable doing dry runs before i strike an arc than I am welding. By the time I feel I have a nice bead going I'm at the end. Lol. here is another picture. At the termination of all the welds I have a black a small spot. Is this normal?
Brian
Looking at this photo I would suggest that the vertical weld be taken a little further into the corner of the joint, then when you finish the horizontal weld, end it right on top of the vertical weld, thereby you'll only see the one stop. This is not a criticism at all, just a suggestion to tie things in and look better.
Richard
Website
Website
- big gear head
-
Ace
-
Posts:
-
Joined:Thu May 07, 2015 11:46 am
-
Location:KY.
I agree, each weld needs to wrap around the corner slightly so that they tie in completely. Start one weld on the end of another and end the weld on another. When you finish a joint it would look like there was only one end to the whole weld.
You can take a file and knock off that black spot before you start your next weld so that it doesn't float along with the next weld. Sometimes that spot can float over to the edge of the weld and get stuck there. While you are welding this spot will look bright red. Try to keep it floating in the puddle all the way to the end of the weld and then you can knock it off.
You can take a file and knock off that black spot before you start your next weld so that it doesn't float along with the next weld. Sometimes that spot can float over to the edge of the weld and get stuck there. While you are welding this spot will look bright red. Try to keep it floating in the puddle all the way to the end of the weld and then you can knock it off.
Freddie
Looks good. Corner tie ins on square tube can take a while because your changing angle and direction at the same time as the heat just sort of soaks the whole piece. And you fight the fact that one side of the joint is usually cut straight and the other is the rounded corner of a tube making for an irregular bevel of sorts.
I have more questions than answers
Josh
Josh
Thanks guys I get what your saying about tying the welds together to look better.
I guess I should have started with a few pictures of my tack welds. I am using .045 70S2 for the tacks and .062 for the welds.
Is this the best way to tack things together when building with square tube?
And here is a progress shot so far.
Brian
I guess I should have started with a few pictures of my tack welds. I am using .045 70S2 for the tacks and .062 for the welds.
Is this the best way to tack things together when building with square tube?
And here is a progress shot so far.
Brian
Brian
Miller Thunderbolt 225 AC/DC
Everlast 255EXT with W300 cooler
Hobo Freight 170 MIG Welder
Miller Thunderbolt 225 AC/DC
Everlast 255EXT with W300 cooler
Hobo Freight 170 MIG Welder
- LtBadd
-
Weldmonger
-
Posts:
-
Joined:Sun Apr 12, 2015 4:00 pm
-
Location:Clearwater FL
-
Contact:
Brian, are you thinking that the .045 will leave a smaller tack which will be easier to consume in the weld? As long as the tacks are enough to keep it together before welding it's a good idea, and it also shows your thinking ahead as well. You're thinking about what you're doing and why, always a good idea, and the traits of a professional.melsdad wrote:Thanks guys I get what your saying about tying the welds together to look better.
I guess I should have started with a few pictures of my tack welds. I am using .045 70S2 for the tacks and .062 for the welds.
Is this the best way to tack things together when building with square tube?
Brian
Richard
Website
Website
LtBad that is exactly what I was thinking. I started out tacking in the center of the tube on another small project. I found it messed up my rytheme when I was dabbing filler metal in and came to the tack in the middle of the bead. When I went to corner tacks I thought it helped with starts and stops of the weld.
Thanks for the compliment!
Brian
Thanks for the compliment!
Brian
Brian
Miller Thunderbolt 225 AC/DC
Everlast 255EXT with W300 cooler
Hobo Freight 170 MIG Welder
Miller Thunderbolt 225 AC/DC
Everlast 255EXT with W300 cooler
Hobo Freight 170 MIG Welder
I am kind of surprised your using 1/16" tungsten at that amperage. I know if I approach that amperage, my tungsten loses it's shape and I go to the 3/32 tungsten. So I kind of use 100 amps as my switch amperage. I do like the 1/16 filler in many cases instead of the 3/32 filler. Your welds look very smooth and steady.
- LtBadd
-
Weldmonger
-
Posts:
-
Joined:Sun Apr 12, 2015 4:00 pm
-
Location:Clearwater FL
-
Contact:
That seems odd...I've used 1/16" right up to 150bruce991 wrote:I am kind of surprised your using 1/16" tungsten at that amperage. I know if I approach that amperage, my tungsten loses it's shape and I go to the 3/32 tungsten. So I kind of use 100 amps as my switch amperage. I do like the 1/16 filler in many cases instead of the 3/32 filler. Your welds look very smooth and steady.
- Attachments
-
- capture20160103081239337.png (39.2 KiB) Viewed 742 times
Richard
Website
Website
GreinTime
- GreinTime
-
Weldmonger
-
Posts:
-
Joined:Fri Nov 01, 2013 11:20 am
-
Location:Pittsburgh, PA
Make sure you have your Arc Force or Hot Start or whatever it's called set to zero. I recall that giving me some funk* issues with my Everlastbruce991 wrote:I am kind of surprised your using 1/16" tungsten at that amperage. I know if I approach that amperage, my tungsten loses it's shape and I go to the 3/32 tungsten. So I kind of use 100 amps as my switch amperage. I do like the 1/16 filler in many cases instead of the 3/32 filler. Your welds look very smooth and steady.
Sent from my SM-G900V using Tapatalk
#oneleggedproblems
-=Sam=-
-=Sam=-
Return to “Tig Welding - Tig Welding Aluminum - Tig Welding Techniques - Aluminum Tig Welding”
Jump to
- Introductions & How to Use the Forum
- ↳ Welcome!
- ↳ Member Introductions
- ↳ How to Use the Forum
- ↳ Moderator Applications
- Welding Discussion
- ↳ Metal Cutting
- ↳ Tig Welding - Tig Welding Aluminum - Tig Welding Techniques - Aluminum Tig Welding
- ↳ Mig and Flux Core - gas metal arc welding & flux cored arc welding
- ↳ Stick Welding/Arc Welding - Shielded Metal Arc Welding
- ↳ Welding Forum General Shop Talk
- ↳ Welding Certification - Stick/Arc Welding, Tig Welding, Mig Welding Certification tests - Welding Tests of all kinds
- ↳ Welding Projects - Welding project Ideas - Welding project plans
- ↳ Product Reviews
- ↳ Fuel Gas Heating
- Welding Tips & Tricks
- ↳ Video Discussion
- ↳ Wish List
- Announcements & Feedback
- ↳ Forum News
- ↳ Suggestions, Feedback and Support
- Welding Marketplace
- ↳ Welding Jobs - Industrial Welding Jobs - Pipe Welding Jobs - Tig Welding Jobs
- ↳ Classifieds - Buy, Sell, Trade Used Welding Equipment
- Welding Resources
- ↳ Tradeshows, Seminars and Events
- ↳ The Welding Library
- ↳ Education Opportunities