Tig welding tips, questions, equipment, applications, instructions, techniques, tig welding machines, troubleshooting tig welding process
duckhunter27
- duckhunter27
-
New Member
-
Posts:
-
Joined:Tue Jan 05, 2016 9:18 pm
Ok guys i need some of your top shelf expertise. When i cap this 4 " stainless schd 10 pipe , im getting some good color but not alot . (No pictures) . Here's the run down miller trailblazer 325d , 26 flexneck torch , 1/8 large gas lens, 2% thoriated tungsten, 12 cup , 30cfh beings im in a basement with a draft . I do have a couple welding screens up . No matter what i tried it wont get any better.
- LtBadd
-
Weldmonger
-
Posts:
-
Joined:Sun Apr 12, 2015 4:00 pm
-
Location:Clearwater FL
-
Contact:
You don't say what color you're getting that you consider "not" good. Color is actually an indication of contamination, straw or gold and blue are considered normal and acceptable.duckhunter27 wrote:Ok guys i need some of your top shelf expertise. When i cap this 4 " stainless schd 10 pipe , im getting some good color but not alot . (No pictures) . Here's the run down miller trailblazer 325d , 26 flexneck torch , 1/8 large gas lens, 2% thoriated tungsten, 12 cup , 30cfh beings im in a basement with a draft . I do have a couple welding screens up . No matter what i tried it wont get any better.
If your getting a gray or darker then that's an indication of a lack of shielding, whether its do to welding too hot or a draft causing a loss of the shielding.
Richard
Website
Website
duckhunter27
- duckhunter27
-
New Member
-
Posts:
-
Joined:Tue Jan 05, 2016 9:18 pm
Sorry about that 80 to 90 amps 3/32 filler rod . Its pretty gray , some have reds and blues with some gold
Don't get too caught up in color, while color is "a" indicator a slight gray color does not mean all is lost.... What does it look like once brushed or pickled?
@Markus
@Markus
I weld stainless, stainless and more stainless...Food Industry, sanitary process piping, vessels, whatever is needed, I like to make stuff.
ASME IX, AWS 17.1, D1.1
Instagram #RNHFAB
ASME IX, AWS 17.1, D1.1
Instagram #RNHFAB
duckhunter27
- duckhunter27
-
New Member
-
Posts:
-
Joined:Tue Jan 05, 2016 9:18 pm
Sounds fine to me then. Post a pic if you can...
I weld stainless, stainless and more stainless...Food Industry, sanitary process piping, vessels, whatever is needed, I like to make stuff.
ASME IX, AWS 17.1, D1.1
Instagram #RNHFAB
ASME IX, AWS 17.1, D1.1
Instagram #RNHFAB
duckhunter27
- duckhunter27
-
New Member
-
Posts:
-
Joined:Tue Jan 05, 2016 9:18 pm
duckhunter27
- duckhunter27
-
New Member
-
Posts:
-
Joined:Tue Jan 05, 2016 9:18 pm
This isn't the cap of course but it looks the exact same . I think its a gas issue. Im running 30 to 45 cfh and can barley feel the gas coming out the lens .
- Attachments
-
- 20160122_140047.jpg (18.55 KiB) Viewed 3123 times
- LtBadd
-
Weldmonger
-
Posts:
-
Joined:Sun Apr 12, 2015 4:00 pm
-
Location:Clearwater FL
-
Contact:
30 to 45 cfh is too much, should be 15 to 20, check for a leak at all connections, or a pin hole in the torch hose.duckhunter27 wrote:This isn't the cap of course but it looks the exact same . I think its a gas issue. Im running 30 to 45 cfh and can barley feel the gas coming out the lens .
Richard
Website
Website
duckhunter27
- duckhunter27
-
New Member
-
Posts:
-
Joined:Tue Jan 05, 2016 9:18 pm
Im in a basement with a pretty good draft . Everytbing is brand new as well torch , all consumables , regulator, gas hose and welding machine. I will try turning it down and check for leaks .
wickedone
- wickedone
-
New Member
-
Posts:
-
Joined:Sat Jan 30, 2016 12:31 pm
-
Location:Spruce Grove Alberta
To Me it looks like you didn't prep the pipe properly before you started. When I do a pressure weld I take all the mill scale off inside and out so I don't drag the scale into the weld. Are you purging the inside??
duckhunter27
- duckhunter27
-
New Member
-
Posts:
-
Joined:Tue Jan 05, 2016 9:18 pm
Yes I'm purging with a purge balloon,also having this problem when doing the tie in , it doesn't seem to want to flow , it just balls up .
- Attachments
-
- image.jpeg (57.75 KiB) Viewed 2867 times
-
- image.jpeg (40.52 KiB) Viewed 2867 times
-
- image.jpeg (36.21 KiB) Viewed 2867 times
- LtBadd
-
Weldmonger
-
Posts:
-
Joined:Sun Apr 12, 2015 4:00 pm
-
Location:Clearwater FL
-
Contact:
It looks like when you stopped you didn't get good gas shielding, so when you resumed the weld the filler didn't want to flow. Perhaps your post flow is too short or you're removing the torch before the weld has cooled.duckhunter27 wrote:Yes I'm purging with a purge balloon,also having this problem when doing the tie in , it doesn't seem to want to flow , it just balls up .
Before starting you'll need to clean this
- Attachments
-
- image.jpeg (76.18 KiB) Viewed 2850 times
Richard
Website
Website
There may be a couple of things that are going on. The contour of the bead seems a bit erratic which could indicate you are struggling with consistent travel speed and controlling the puddle.
I would concentrate more on the shape/appearance of that weld more than the "color".
Get in a position is which you can move the torch around the pipe comfortable and consistently, even if its just for a 30-60 degree section.
Just an opinion to add to some of the other good ones provided.
I would concentrate more on the shape/appearance of that weld more than the "color".
Get in a position is which you can move the torch around the pipe comfortable and consistently, even if its just for a 30-60 degree section.
Just an opinion to add to some of the other good ones provided.
Gerald Austin
If I didn't say it in the post- Have a great day !
Greeneville Tn
If I didn't say it in the post- Have a great day !
Greeneville Tn
Now that I see some other pictures, removing the oxide layer from around your weld area can also help with the bead wetting out. Clean em up some if you are looking to improve the appearance.
Gerald Austin
If I didn't say it in the post- Have a great day !
Greeneville Tn
If I didn't say it in the post- Have a great day !
Greeneville Tn
duckhunter27
- duckhunter27
-
New Member
-
Posts:
-
Joined:Tue Jan 05, 2016 9:18 pm
after I stop I leave the torch on the weld till the area isn't glowing red any longer , I'm using a 26 style flex neck with a valve so it pouring gas at a rate of about 45 to 50 Cfh due to I'm in an extremely drafty basement , thanks again for all the adviceLtBadd wrote:It looks like when you stopped you didn't get good gas shielding, so when you resumed the weld the filler didn't want to flow. Perhaps your post flow is too short or you're removing the torch before the weld has cooled.duckhunter27 wrote:Yes I'm purging with a purge balloon,also having this problem when doing the tie in , it doesn't seem to want to flow , it just balls up .
Before starting you'll need to clean this
That is a little weird, I can see a pretty consistent walking pattern, then it goes into the weirdness. What's the purge pressure?
Looks like the torch angle is off in that area. Is it always the same position on the piping?
Looks like the torch angle is off in that area. Is it always the same position on the piping?
I weld stainless, stainless and more stainless...Food Industry, sanitary process piping, vessels, whatever is needed, I like to make stuff.
ASME IX, AWS 17.1, D1.1
Instagram #RNHFAB
ASME IX, AWS 17.1, D1.1
Instagram #RNHFAB
duckhunter27
- duckhunter27
-
New Member
-
Posts:
-
Joined:Tue Jan 05, 2016 9:18 pm
Rick H it's generally where there is a a stop and start at , i wish I could video it for you guys to show you . It literally looks like it balls up and doesn't want to flow in just ball up . The purge pressure is around 10 to 15 . Yes always same position, I'm sure it's the operator and not material just wanna figure it out before it drives me insane lol .
Once you have the joint almost welded you could probably back down on the purge. I've had a few times I've had someone actually shut the purge off just before I close the last of the gap.
I have more questions than answers
Josh
Josh
Poland308 wrote:Once you have the joint almost welded you could probably back down on the purge. I've had a few times I've had someone actually shut the purge off just before I close the last of the gap.
Kinda my thoughts too but depending on the length of the pipe and vent hole those flow #s don't seem to far off. Ive had to back my purge down on some sanitary stuff for the same reason, but its no filler. Since this is pipe with a root, fill and cap I'm skeptical the purge is the issue but figured Id touch all bases..lol
Since it is where a start and stop is maybe its contamination but the weld doesn't look horrible. If you are brushing well try running past your start/stop another 1/2" or so and see if it follows.
I weld stainless, stainless and more stainless...Food Industry, sanitary process piping, vessels, whatever is needed, I like to make stuff.
ASME IX, AWS 17.1, D1.1
Instagram #RNHFAB
ASME IX, AWS 17.1, D1.1
Instagram #RNHFAB
Return to “Tig Welding - Tig Welding Aluminum - Tig Welding Techniques - Aluminum Tig Welding”
Jump to
- Introductions & How to Use the Forum
- ↳ Welcome!
- ↳ Member Introductions
- ↳ How to Use the Forum
- ↳ Moderator Applications
- Welding Discussion
- ↳ Metal Cutting
- ↳ Tig Welding - Tig Welding Aluminum - Tig Welding Techniques - Aluminum Tig Welding
- ↳ Mig and Flux Core - gas metal arc welding & flux cored arc welding
- ↳ Stick Welding/Arc Welding - Shielded Metal Arc Welding
- ↳ Welding Forum General Shop Talk
- ↳ Welding Certification - Stick/Arc Welding, Tig Welding, Mig Welding Certification tests - Welding Tests of all kinds
- ↳ Welding Projects - Welding project Ideas - Welding project plans
- ↳ Product Reviews
- ↳ Fuel Gas Heating
- Welding Tips & Tricks
- ↳ Video Discussion
- ↳ Wish List
- Announcements & Feedback
- ↳ Forum News
- ↳ Suggestions, Feedback and Support
- Welding Marketplace
- ↳ Welding Jobs - Industrial Welding Jobs - Pipe Welding Jobs - Tig Welding Jobs
- ↳ Classifieds - Buy, Sell, Trade Used Welding Equipment
- Welding Resources
- ↳ Tradeshows, Seminars and Events
- ↳ The Welding Library
- ↳ Education Opportunities