Hi all.
So i'm looking for some advice, i've always mig welded stainless so tig is a bit new to me
My setup is as follows:
Eastwood tig 200
Argon set to roughly 8LPM-4LPM roughly 15cfh- No flowmeter ATM other than bottles built in regulator, and converting units from uk to usa for easy reading for people.
Running 40amps
0.2sec pre-flow
4sec post-flow
Number 6 cup - no gas lense
No back purge
Foot pedal not used
Using 1.6mm or 1/16 2% thoriated tungstens ground to quite a sharp point
1.6mm or 1/16 308L filler rod
Practicing beads on some 304L stainless 1.5mm or 0.060 wall thickness pipe i had laying about.
Now i wasnt surgically clean in my prep, only scotchbrite pad till clean in places. Some places i did not bother at all so i knew what dirty and clean welded like.
Here's a picture of the best welds i could manage in around 1.5hours before i got hungry and went in search for food.
Weirdly enough my spot welds came out quite nice color when i used 60-80amps and survived a good hammer test
Just looking for advice and tips on getting coloring as atm mine are looking quite gray, found what i can find using google and search buttons i believe a longer post flow, gas lense and back purge will help?
Would using a smaller filler rod mean i could move quicker? if so could i use the stainless mig wire on the reel i have left?
thanks for any replys it means a lot i'll try to not annoy with silly questions
Tig welding tips, questions, equipment, applications, instructions, techniques, tig welding machines, troubleshooting tig welding process
- Braehill
-
Weldmonger
-
Posts:
-
Joined:Sat Jul 06, 2013 11:16 am
-
Location:Near Pittsburgh,Pennsylvania. Steel Buckle of the Rust Belt
fordy,
First off welcome to the forum, feel free to use the introduction page and tell us a little about yourself.
The simple answer to all your questions is yes.
The long answer is, yes you can use the thin Mig wire you have. The more you practice on the same piece, the more it will turn gray due to overheating. A gas lens will help with color, as will a back purge. You can also bump up your post flow and hold it there until it ends.
Len
First off welcome to the forum, feel free to use the introduction page and tell us a little about yourself.
The simple answer to all your questions is yes.
The long answer is, yes you can use the thin Mig wire you have. The more you practice on the same piece, the more it will turn gray due to overheating. A gas lens will help with color, as will a back purge. You can also bump up your post flow and hold it there until it ends.
Len
Now go melt something.
Instagram @lenny_gforce
Len
Instagram @lenny_gforce
Len
Personally I'd increase to 55-60 amps and move faster, will also help wet out the 1/16" filler. Or you could try 40amp with .030-.035" mig filler. I'd say your post flow is on par for 40amps.
That small piece of tubing has just gotten heat soaked I believe that is why some of the welds are very grey, and being at only ,40amps it took to long to melt the filler properly.
The back purge will only help with backside sugaring, it will not do much for your front side.
That small piece of tubing has just gotten heat soaked I believe that is why some of the welds are very grey, and being at only ,40amps it took to long to melt the filler properly.
The back purge will only help with backside sugaring, it will not do much for your front side.
I weld stainless, stainless and more stainless...Food Industry, sanitary process piping, vessels, whatever is needed, I like to make stuff.
ASME IX, AWS 17.1, D1.1
Instagram #RNHFAB
ASME IX, AWS 17.1, D1.1
Instagram #RNHFAB
Thanks for replied guys
I tried higher ampages but I couldn't move fast enough and the weld went really flat.
I admit that was when I was playing around trying to get comfortable at the beginning with my torch angle/movement and filler dabbing is pants
Found last night doing research that when the filler rod balls up its because the torch angle is wrong
I noticed when I raised the amps the weld behind the pool just went really dark and flakey grey I did think possibly gas shield but never thought about the heat in the piece...I'll have to keep an eye on that
I've ordered a gas lense no 6 + 8 1/16 and flow meter so will try again when they turn up
I tried higher ampages but I couldn't move fast enough and the weld went really flat.
I admit that was when I was playing around trying to get comfortable at the beginning with my torch angle/movement and filler dabbing is pants
Found last night doing research that when the filler rod balls up its because the torch angle is wrong
I noticed when I raised the amps the weld behind the pool just went really dark and flakey grey I did think possibly gas shield but never thought about the heat in the piece...I'll have to keep an eye on that
I've ordered a gas lense no 6 + 8 1/16 and flow meter so will try again when they turn up
Return to “Tig Welding - Tig Welding Aluminum - Tig Welding Techniques - Aluminum Tig Welding”
Jump to
- Introductions & How to Use the Forum
- ↳ Welcome!
- ↳ Member Introductions
- ↳ How to Use the Forum
- ↳ Moderator Applications
- Welding Discussion
- ↳ Metal Cutting
- ↳ Tig Welding - Tig Welding Aluminum - Tig Welding Techniques - Aluminum Tig Welding
- ↳ Mig and Flux Core - gas metal arc welding & flux cored arc welding
- ↳ Stick Welding/Arc Welding - Shielded Metal Arc Welding
- ↳ Welding Forum General Shop Talk
- ↳ Welding Certification - Stick/Arc Welding, Tig Welding, Mig Welding Certification tests - Welding Tests of all kinds
- ↳ Welding Projects - Welding project Ideas - Welding project plans
- ↳ Product Reviews
- ↳ Fuel Gas Heating
- Welding Tips & Tricks
- ↳ Video Discussion
- ↳ Wish List
- Announcements & Feedback
- ↳ Forum News
- ↳ Suggestions, Feedback and Support
- Welding Marketplace
- ↳ Welding Jobs - Industrial Welding Jobs - Pipe Welding Jobs - Tig Welding Jobs
- ↳ Classifieds - Buy, Sell, Trade Used Welding Equipment
- Welding Resources
- ↳ Tradeshows, Seminars and Events
- ↳ The Welding Library
- ↳ Education Opportunities