WPS for TIG states; Current and Polarity, dc, -ve to torch and I haven't seen that before. I'm doing stainless, so dc-.
It also lists Arc energy range to 2.5 kj/mm and Voltage range of 11-12V? Both of which I've never seen when talking TIG.
Tig welding tips, questions, equipment, applications, instructions, techniques, tig welding machines, troubleshooting tig welding process
- weldin mike 27
-
Weldmonger
-
Posts:
-
Joined:Fri Apr 01, 2011 10:59 pm
-
Location:Australia; Victoria
Kj/mm refers to your travel speed for a given setting. For tightly controlled heat input. On some ss it is ruined if held above a certain temp for too long.
- Otto Nobedder
-
Weldmonger
-
Posts:
-
Joined:Thu Jan 06, 2011 11:40 pm
-
Location:Near New Orleans
Yes.gnabgib wrote:Thanks and is dc,-ve to torch possibly just a technical way of saying dc-?
Some newbie weld engineer was trying to use his new vocabulary. All he really said was, "DC-"
Steve S
Ha!..Thanks Steve, confirms my suspicions. Thinks...Must remember to read between the lines.Otto Nobedder wrote:Yes.gnabgib wrote:Thanks and is dc,-ve to torch possibly just a technical way of saying dc-?
Some newbie weld engineer was trying to use his new vocabulary. All he really said was, "DC-"
Steve S
Jeff
- weldin mike 27
-
Weldmonger
-
Posts:
-
Joined:Fri Apr 01, 2011 10:59 pm
-
Location:Australia; Victoria
There should be given the amperage range to follow. For example 70-90 A. That kj/mm is heat input and it's bit weird that it is given if amps are not.
Voltage does affect to the heat input as well, but usually that is not given for hand welding due to change of your tungstens hight. 10 volts refers to very small cap between workpiece and tungsten. Couple of mils or so.
Also how to determine your welding speed and track that in every single weld? Impossible with hand welding...
Voltage does affect to the heat input as well, but usually that is not given for hand welding due to change of your tungstens hight. 10 volts refers to very small cap between workpiece and tungsten. Couple of mils or so.
Also how to determine your welding speed and track that in every single weld? Impossible with hand welding...
-Markus-
I was given all the details including the amperage range and travel speed, I just haven't included all of that here.Markus wrote:There should be given the amperage range to follow. For example 70-90 A. That kj/mm is heat input and it's bit weird that it is given if amps are not.
Voltage does affect to the heat input as well, but usually that is not given for hand welding due to change of your tungstens hight. 10 volts refers to very small cap between workpiece and tungsten. Couple of mils or so.
Also how to determine your welding speed and track that in every single weld? Impossible with hand welding...
- TRACKRANGER
-
Weldmonger
-
Posts:
-
Joined:Wed Aug 06, 2014 12:48 am
-
Location:Melbourne, Australia
It would be great to see all of the settings. Might put everything into perspective a little better for others to follow.gnabgib wrote:
I was given all the details including the amperage range and travel speed, I just haven't included all of that here.
Thanks
Trevor
EWM Phonenix 355 Pulse MIG set mainly for Aluminum, CIGWeld 300Amp AC/DC TIG, TRANSMIG S3C 300 Amp MIG, etc, etc
Well, the procedure was supplied 'In confidence' so if I gave you all the details I might have to kill youTRACKRANGER wrote:It would be great to see all of the settings. Might put everything into perspective a little better for others to follow.gnabgib wrote:
I was given all the details including the amperage range and travel speed, I just haven't included all of that here.
Thanks
Trevor
- Otto Nobedder
-
Weldmonger
-
Posts:
-
Joined:Thu Jan 06, 2011 11:40 pm
-
Location:Near New Orleans
That said, the Kj/mm is an upper heat limit, or travel-speed quantity, as was mentioned by another. Just stick with the WPS amps, and move fast enough you don't make it black, and you should be fine.gnabgib wrote:Well, the procedure was supplied 'In confidence' so if I gave you all the details I might have to kill youTRACKRANGER wrote:It would be great to see all of the settings. Might put everything into perspective a little better for others to follow.gnabgib wrote:
I was given all the details including the amperage range and travel speed, I just haven't included all of that here.
Thanks
Trevor
Steve S
That said, the Kj/mm is an upper heat limit, or travel-speed quantity, as was mentioned by another. Just stick with the WPS amps, and move fast enough you don't make it black, and you should be fine.
Steve S[/quote]
Thanks, but I have to admit it's got me in a knot and I'm thinking now of making a micro rotator, because of the small size and it being a critical weld.
Jeff
Steve S[/quote]
Thanks, but I have to admit it's got me in a knot and I'm thinking now of making a micro rotator, because of the small size and it being a critical weld.
Jeff
- Otto Nobedder
-
Weldmonger
-
Posts:
-
Joined:Thu Jan 06, 2011 11:40 pm
-
Location:Near New Orleans
If you build that "micro-rotator", please share what you build!
I envision a variable-speed geared electric drill (Max 500 RPM, DeWalt makes one) with the trigger replaced with a potentiometer, for speeds as low as 5 RPM, clamped in a vise.
Without knowing the specifics of your project, this is the cheapest accurate rotator I can imagine.
Steve S
I envision a variable-speed geared electric drill (Max 500 RPM, DeWalt makes one) with the trigger replaced with a potentiometer, for speeds as low as 5 RPM, clamped in a vise.
Without knowing the specifics of your project, this is the cheapest accurate rotator I can imagine.
Steve S
- weldin mike 27
-
Weldmonger
-
Posts:
-
Joined:Fri Apr 01, 2011 10:59 pm
-
Location:Australia; Victoria
Sewing machine motor. Already has a foot control, and lots are connected via belts and not built in. So easy to adapt.
I'll probably get a geared 12v servo motor, with maybe 5rpm at the shaft and gear accordingly. Need up to 26mm per minute but next question is that of the return contact. Maybe a small copper arm, spring loaded to maintain contact while the work piece is turning. I think I have the purge attachment worked out.
- MinnesotaDave
-
Weldmonger
-
Posts:
-
Joined:Sun Oct 27, 2013 10:57 pm
-
Location:Big Lake/Monticello MN, U.S.A.
A little back ground on heat input may help you determine your speed needed for your weld positioner.
Just solve for "S"
Just solve for "S"
- heat input Kj.GIF (29.01 KiB) Viewed 523 times
Dave J.
Beware of false knowledge; it is more dangerous than ignorance. ~George Bernard Shaw~
Syncro 350
Invertec v250-s
Thermal Arc 161 and 300
MM210
Dialarc
Tried being normal once, didn't take....I think it was a Tuesday.
Beware of false knowledge; it is more dangerous than ignorance. ~George Bernard Shaw~
Syncro 350
Invertec v250-s
Thermal Arc 161 and 300
MM210
Dialarc
Tried being normal once, didn't take....I think it was a Tuesday.
- TRACKRANGER
-
Weldmonger
-
Posts:
-
Joined:Wed Aug 06, 2014 12:48 am
-
Location:Melbourne, Australia
"Up to 26mm per minute"?gnabgib wrote:I'll probably get a geared 12v servo motor, with maybe 5rpm at the shaft and gear accordingly. Need up to 26mm per minute but next question is that of the return contact. Maybe a small copper arm, spring loaded to maintain contact while the work piece is turning. I think I have the purge attachment worked out.
Just asking. Are you sure that's not missing a zero or something?
If it was e.g. 12mm diameter rotating at 5 RPM, the travel distance would be at least 188 mm per minute.
To get 26mm per minute with a 12mm diameter job, you would need a rotation speed of ~0.7 RPM. While I don't know the diameter being used, it somehow seems awful slow.
This 'secret' job is getting more and more intriguing ...
Trev
EWM Phonenix 355 Pulse MIG set mainly for Aluminum, CIGWeld 300Amp AC/DC TIG, TRANSMIG S3C 300 Amp MIG, etc, etc
Return to “Tig Welding - Tig Welding Aluminum - Tig Welding Techniques - Aluminum Tig Welding”
Jump to
- Introductions & How to Use the Forum
- ↳ Welcome!
- ↳ Member Introductions
- ↳ How to Use the Forum
- ↳ Moderator Applications
- Welding Discussion
- ↳ Metal Cutting
- ↳ Tig Welding - Tig Welding Aluminum - Tig Welding Techniques - Aluminum Tig Welding
- ↳ Mig and Flux Core - gas metal arc welding & flux cored arc welding
- ↳ Stick Welding/Arc Welding - Shielded Metal Arc Welding
- ↳ Welding Forum General Shop Talk
- ↳ Welding Certification - Stick/Arc Welding, Tig Welding, Mig Welding Certification tests - Welding Tests of all kinds
- ↳ Welding Projects - Welding project Ideas - Welding project plans
- ↳ Product Reviews
- ↳ Fuel Gas Heating
- Welding Tips & Tricks
- ↳ Video Discussion
- ↳ Wish List
- Announcements & Feedback
- ↳ Forum News
- ↳ Suggestions, Feedback and Support
- Welding Marketplace
- ↳ Welding Jobs - Industrial Welding Jobs - Pipe Welding Jobs - Tig Welding Jobs
- ↳ Classifieds - Buy, Sell, Trade Used Welding Equipment
- Welding Resources
- ↳ Tradeshows, Seminars and Events
- ↳ The Welding Library
- ↳ Education Opportunities