Hobby welder, new to tig here and making my welding table.
I will be tig welding 2 - 1/8" 2 X 2 Tubes together and would like a full penetration weld for strenght. I will use a 1/16 or 3/32 rod to leave a gap. Do I need to bevel, or will I be ok with this small thickness. I have done a few practice butt welds with a gap and seemed to have a good amount of metal on the backside when done. Also, Can I do this in one pass or should I be doing a root pass and a cap of some sort. My practice runs seem to look pretty good with one pass.
Thanks
Tig welding tips, questions, equipment, applications, instructions, techniques, tig welding machines, troubleshooting tig welding process
I TIG and MIG 11ga 2x2 tube structures almost each week. I always cut a bevel to about 1/16" land. No gap. Single pass almost always, unless I need to get up over a corner roll on some joints.
The bevel is a good habit I think, but not completely necessary based on your application.
Putting in a root gap as you mentioned is advanced welding, and completely unnecessary for you to do when building a welding table....unless you want the practice of doing it.
The bevel is a good habit I think, but not completely necessary based on your application.
Putting in a root gap as you mentioned is advanced welding, and completely unnecessary for you to do when building a welding table....unless you want the practice of doing it.
Gap or not, you can get all the penetration you need with your TIG. What is more beneficial is to actually clean the inside of the tubing where you butt the weld. If you gap, and don't clean it, you're sucking all that mill scale, grime and crap into your puddle. Take a Dremel and clean back about an inch.
Gap it with 0.035 MIG wire (2 pieces, bent into Vs to spread the tubing). Tack it using 3/32 filler. Jerk the MIG wire out. Take your time and stuff the filler in as you go making sure to get the filler INTO the puddle, not ahead of the puddle. You will have a fully penetrated weld that you can blend down on the outside without losing strength.
Gap it with 0.035 MIG wire (2 pieces, bent into Vs to spread the tubing). Tack it using 3/32 filler. Jerk the MIG wire out. Take your time and stuff the filler in as you go making sure to get the filler INTO the puddle, not ahead of the puddle. You will have a fully penetrated weld that you can blend down on the outside without losing strength.
Thanks for the guidance on this. I have a Primeweld 225, so plenty of amps. I have been using 120 for all of my practice and plan to use that for this also. I think I will experiment with both the 035 gap and the bevel with land on these. Figure it is more good practice. On some of my practice butt joints that were pushed against each other with no bevel, I was not seeing full penetration on the back side; Likely due to my inexperience. I was seeing some, just not the whole weld.
Return to “Tig Welding - Tig Welding Aluminum - Tig Welding Techniques - Aluminum Tig Welding”
Jump to
- Introductions & How to Use the Forum
- ↳ Welcome!
- ↳ Member Introductions
- ↳ How to Use the Forum
- ↳ Moderator Applications
- Welding Discussion
- ↳ Metal Cutting
- ↳ Tig Welding - Tig Welding Aluminum - Tig Welding Techniques - Aluminum Tig Welding
- ↳ Mig and Flux Core - gas metal arc welding & flux cored arc welding
- ↳ Stick Welding/Arc Welding - Shielded Metal Arc Welding
- ↳ Welding Forum General Shop Talk
- ↳ Welding Certification - Stick/Arc Welding, Tig Welding, Mig Welding Certification tests - Welding Tests of all kinds
- ↳ Welding Projects - Welding project Ideas - Welding project plans
- ↳ Product Reviews
- ↳ Fuel Gas Heating
- Welding Tips & Tricks
- ↳ Video Discussion
- ↳ Wish List
- Announcements & Feedback
- ↳ Forum News
- ↳ Suggestions, Feedback and Support
- Welding Marketplace
- ↳ Welding Jobs - Industrial Welding Jobs - Pipe Welding Jobs - Tig Welding Jobs
- ↳ Classifieds - Buy, Sell, Trade Used Welding Equipment
- Welding Resources
- ↳ Tradeshows, Seminars and Events
- ↳ The Welding Library
- ↳ Education Opportunities