I go to a technical school for welding an I'm havering trouble with smaw on 5g pipe. When I weld from the 6 o'clock to the 9 o'clock position my penatration on my root pass comes out flat instead of a crown. Dose anyone have any advise for me on how I can at least get it to crown?
The spacifices are 6 inch diameter pipe 3/8 thick. My root opening is a 1/8 inch an my land is a 1/8 inch. An the welding machine is a Lincoln invertec v350-pro. An the electrode is 1/8 fleetwood 5p+ (6010)
Stick Welding Tips, Certification tests, machines, projects
- Otto Nobedder
-
Weldmonger
-
Posts:
-
Joined:Thu Jan 06, 2011 11:40 pm
-
Location:Near New Orleans
1/8" 5P is the right rod for the job.
I do this weld quite hot, compared to most people. I like 105A, and once the puddle is established on the tack, and the rod is hot (doesn't take long... ), I jamb the rod into the root opening like I'm trying to force it through, and drag the rod (it's still 90 degrees to the pipe... "pull" might be a better word.)
The arc is almost entirely inside the pipe. It sounds like a hive of pissed-off bees. I can raise my hood. There's very little light or arc spray outside the pipe.
It works because the flux insulates the rod from the edges of the land at the bottom of the bevel.
This works at 95A, too, but I like 105 because I can go to 1/8" 7018 without adjusting the machine.
Here's one done that way on 8" sch 80, in 5G (root wire-wheeled for the camera):
Steve S
I do this weld quite hot, compared to most people. I like 105A, and once the puddle is established on the tack, and the rod is hot (doesn't take long... ), I jamb the rod into the root opening like I'm trying to force it through, and drag the rod (it's still 90 degrees to the pipe... "pull" might be a better word.)
The arc is almost entirely inside the pipe. It sounds like a hive of pissed-off bees. I can raise my hood. There's very little light or arc spray outside the pipe.
It works because the flux insulates the rod from the edges of the land at the bottom of the bevel.
This works at 95A, too, but I like 105 because I can go to 1/8" 7018 without adjusting the machine.
Here's one done that way on 8" sch 80, in 5G (root wire-wheeled for the camera):
Steve S
Joe the welder
- Joe the welder
-
New Member
-
Posts:
-
Joined:Wed Nov 28, 2012 3:43 pm
- Otto Nobedder
-
Weldmonger
-
Posts:
-
Joined:Thu Jan 06, 2011 11:40 pm
-
Location:Near New Orleans
Yes. 1/8" root opening (it closes slightly as it draws), and the land on that weld was closer to 3/32".
Steve S
Steve S
Joe the welder
- Joe the welder
-
New Member
-
Posts:
-
Joined:Wed Nov 28, 2012 3:43 pm
Return to “Stick Welding/Arc Welding - Shielded Metal Arc Welding”
Jump to
- Introductions & How to Use the Forum
- ↳ Welcome!
- ↳ Member Introductions
- ↳ How to Use the Forum
- ↳ Moderator Applications
- Welding Discussion
- ↳ Metal Cutting
- ↳ Tig Welding - Tig Welding Aluminum - Tig Welding Techniques - Aluminum Tig Welding
- ↳ Mig and Flux Core - gas metal arc welding & flux cored arc welding
- ↳ Stick Welding/Arc Welding - Shielded Metal Arc Welding
- ↳ Welding Forum General Shop Talk
- ↳ Welding Certification - Stick/Arc Welding, Tig Welding, Mig Welding Certification tests - Welding Tests of all kinds
- ↳ Welding Projects - Welding project Ideas - Welding project plans
- ↳ Product Reviews
- ↳ Fuel Gas Heating
- Welding Tips & Tricks
- ↳ Video Discussion
- ↳ Wish List
- Announcements & Feedback
- ↳ Forum News
- ↳ Suggestions, Feedback and Support
- Welding Marketplace
- ↳ Welding Jobs - Industrial Welding Jobs - Pipe Welding Jobs - Tig Welding Jobs
- ↳ Classifieds - Buy, Sell, Trade Used Welding Equipment
- Welding Resources
- ↳ Tradeshows, Seminars and Events
- ↳ The Welding Library
- ↳ Education Opportunities