Stick Welding Tips, Certification tests, machines, projects
Trying to build a desk for my wife. Getting a lot of porosity and don’t know why. On my ranger 10000, the amps are set to 90 and the dial all the way to just above five. These are new off the shelf electrodes. I am holding a tight arc and good to me travel speed. I also have a bad wrack to it. All the cuts are dead nuts on. I put the gussets on the bottom frame prior to welding the legs to the top frame and I think it’s putting strain on it not allowing it to level out. Can I get some help. I can upload more pics if necessary when I get home in a few.
- Attachments
-
- The frame in all its glory:/
- 847998FA-89B7-43D6-8AE8-579AB62C3CC0.jpeg (57.86 KiB) Viewed 2219 times
- MinnesotaDave
-
Weldmonger
-
Posts:
-
Joined:Sun Oct 27, 2013 10:57 pm
-
Location:Big Lake/Monticello MN, U.S.A.
Normally on DC those are run DCEP
Around 90-100 amps is where I usually run 3/32" 7018.
Sometimes as low as 85 amps.
edit: I looked up your machine. You're set on the 40-90 amp range so you're only at about 65 amps or so. Pretty low for 3/32" 7018.
Around 90-100 amps is where I usually run 3/32" 7018.
Sometimes as low as 85 amps.
edit: I looked up your machine. You're set on the 40-90 amp range so you're only at about 65 amps or so. Pretty low for 3/32" 7018.
Dave J.
Beware of false knowledge; it is more dangerous than ignorance. ~George Bernard Shaw~
Syncro 350
Invertec v250-s
Thermal Arc 161 and 300
MM210
Dialarc
Tried being normal once, didn't take....I think it was a Tuesday.
Beware of false knowledge; it is more dangerous than ignorance. ~George Bernard Shaw~
Syncro 350
Invertec v250-s
Thermal Arc 161 and 300
MM210
Dialarc
Tried being normal once, didn't take....I think it was a Tuesday.
Thanks for the prompt reply Dave. I appreciate the information and will make the changes. I move the amperage down due to the fact that I kept blowing through this material is less than 1/8 inch thick so I was trying to keep from blowing through. I will adjust my technique and try it with the higher amperage. I am getting good penetration however, But with a lot of porosity.
Farmwelding
- Farmwelding
-
Weldmonger
-
Posts:
-
Joined:Thu Mar 10, 2016 11:37 pm
-
Location:Wisconsin
Have any pictures of the porosity and the electrodes? Have they been exposed to a lot of moisture?
A student now but really want to weld everyday. Want to learn everything about everything. Want to become a knower of all and master of none.
Instagram: @farmwelding
Nick
Instagram: @farmwelding
Nick
Farm welding, I will get some pictures when I get home. As I said in my original post, these are brand new electrodea so I have no idea what their exposure has been. I bought them at Lowe’s so anything is possible.
Ok here is a pic of a little porosity and yes, under cut. Also a pic of the thickness. I believe it it just over 1/16”
- Attachments
-
- CAFC1A91-0709-49CD-AE70-435BAEEDA9CA.jpeg (27.22 KiB) Viewed 2200 times
-
- 05BA5510-107F-493C-B5FF-51604949A91D.jpeg (34.92 KiB) Viewed 2200 times
.Poland308 wrote:Are you getting porosity only on the last weld that is sealing up the tube? Oil contamination will also cause holes like that.
I didn’t use acetone to clean it but I tried to make sure it was bright shiny metal. Just clarify though, this was scrap metal from my neighbor. Maybe there was something on it although there didn’t appear to be.
On real thin 1/8 or less I’d personally run a little colder than Dave. Just personally. I’d be at about 70-80. If there is any oily residue on the inside of the tube then it will get pulled through the molten pool as you weld. This can definitely cause porosity. Some kinds of Left over paint or any kind of zinc/galvanizing, same thing. If you weld the pipe or tube totally closed and don’t allow for hot air to escape then this can cause porosity as well, but usually only as your making the last stretch of weld. Rod condition is less likely. I have some 7018 that got rained on, the iron powder in the flux actually has started to rust. I use it for lots of non essential stuff with no porosity. However if the flux is soaked in oil, water, glycol, or cracking and flaking off in chunks either before or during a weld then it’s worthless and will also cause holes.
I have more questions than answers
Josh
Josh
Ok so, I changed to AC and bumped the amps to 65 or so. There is still a little porosity but not as bad as it was before. Still sticking a lot whic I think is indicative of low amps but I don’t eat to burn through. I appreciate all your help. I will post a pic of the final product.
Return to “Stick Welding/Arc Welding - Shielded Metal Arc Welding”
Jump to
- Introductions & How to Use the Forum
- ↳ Welcome!
- ↳ Member Introductions
- ↳ How to Use the Forum
- ↳ Moderator Applications
- Welding Discussion
- ↳ Metal Cutting
- ↳ Tig Welding - Tig Welding Aluminum - Tig Welding Techniques - Aluminum Tig Welding
- ↳ Mig and Flux Core - gas metal arc welding & flux cored arc welding
- ↳ Stick Welding/Arc Welding - Shielded Metal Arc Welding
- ↳ Welding Forum General Shop Talk
- ↳ Welding Certification - Stick/Arc Welding, Tig Welding, Mig Welding Certification tests - Welding Tests of all kinds
- ↳ Welding Projects - Welding project Ideas - Welding project plans
- ↳ Product Reviews
- ↳ Fuel Gas Heating
- Welding Tips & Tricks
- ↳ Video Discussion
- ↳ Wish List
- Announcements & Feedback
- ↳ Forum News
- ↳ Suggestions, Feedback and Support
- Welding Marketplace
- ↳ Welding Jobs - Industrial Welding Jobs - Pipe Welding Jobs - Tig Welding Jobs
- ↳ Classifieds - Buy, Sell, Trade Used Welding Equipment
- Welding Resources
- ↳ Tradeshows, Seminars and Events
- ↳ The Welding Library
- ↳ Education Opportunities